The complaint usually arrives as a quality issue: a batch of potted modules with a tacky surface, or a casting that feels soft in the middle. The resin supplier is called first, then the hardener. In most cases the material is fine and the machine has been quietly running at the wrong ratio.
Three symptoms, one root cause
Ratio drift does not announce itself. It appears as a surface that stays tacky for days, a casting that cures hard on the outside and soft inside, or a batch that passes in summer and fails in winter. All three point to the same thing: the actual mix is not the mix on the HMI.
A ±2% metering tolerance sounds tight, but on a 100:10 system a 2% error in the hardener stream is a 20% error in the curing agent. Ratio accuracy has to be read relative to the smaller component, not the total.
Cause one: pump wear from filled material
Gear pumps are precise until the material contains an abrasive filler. Aluminium oxide, boron nitride and silica fillers slowly open the clearances, and an opened clearance leaks material past the gears instead of displacing it. The pump still turns, the pressure still reads normal, and the ratio quietly falls.
Hardened screw or progressive-cavity pumps with wear-compensating seals last longer on filled systems. Either way, pump displacement needs periodic verification against a weighed sample — a five-minute check that prevents a month of scrap.
Cause two: viscosity difference meeting temperature change
Component A is often three to five times more viscous than component B. Flow through the same restriction therefore responds differently to temperature. A workshop that is 12 °C colder in winter changes both viscosities, but not by the same amount, so the ratio moves.
This is why tank heating and line temperature control are not optional on high-ratio systems. It is also why a machine that was calibrated in July should be re-checked in January.
Cause three: back pressure changing between shots
When the mixing head discharges into a narrow cavity or a long nozzle, back pressure rises. If the two streams see different back pressures — because of different line lengths or a partially blocked static mixer — the lower-viscosity stream wins. The ratio shifts exactly when the part geometry changes.
Pressure feedback on both lines, not just the mixed outlet, is the practical way to see this. It is also the reason a machine that potted large housings perfectly can fail on a small, deep cavity.
One test that separates machine from material
Run a timed shot into a tared cup with the mixing element removed, weighing each component separately. Compare the measured masses against the programmed ratio. If the masses are correct but the cured part is not, the problem is mixing or the material. If the masses are wrong, the problem is the machine.
This test takes ten minutes and settles the argument. Without it, both the resin supplier and the equipment builder will keep pointing at each other.
Key points
- Read ratio accuracy against the smaller component, not the total.
- Abrasive fillers wear gear pumps invisibly — verify displacement by weight.
- Temperature changes shift high-ratio systems more than low-ratio ones.
- Weigh each component separately before blaming the resin.